A failed bend test on a procedure qualification record is painful. The coupon has been welded, cut and machined, the inspector has signed off on the parameters, and then a crack opens up on the convex face of the bend. Now you’re welding the whole thing again.
We test a lot of PQR and welder qualification coupons, and the failures tend to have the same handful of causes. Most of them are avoidable.
What the bend test is actually checking
A guided bend stretches the weld and heat-affected zone well past yield. Sound metal stretches. Lack of fusion, slag and porosity don’t – they open up. Under ASME Section IX the usual acceptance rule is that no open discontinuity on the convex surface may exceed 3 mm (1/8 in) in any direction, with some allowance for cracks at the corners of the specimen. AWS D1.1 has similar but not identical rules, so check which code you’re working to.
The usual causes of failure
Lack of sidewall fusion
This is the big one, especially in side bends on thicker plate. Side bends are required for thicker coupons – under ASME IX, from 19 mm (3/4 in) – and they’re very good at finding fill passes that didn’t wet into the bevel face. Narrow bevel angles, too little travel angle and too-low current on fill passes are the common culprits.
Slag trapped between passes
With SMAW and flux-cored processes, slag left in the toe of a previous pass gets buried by the next one. Proper interpass cleaning and grinding of sharp toes stops most of it.
Root problems
Root bends expose incomplete penetration and suck-back. Root opening, land and alignment need to be right before the first bead goes in. This is why fit-up inspection is worth doing on a qualification coupon.
Specimen preparation
Not every failure is a welding failure. Weld reinforcement must be removed flush, grinding marks should run along the specimen rather than across it, and sharp edges need a small radius. A deep transverse grinding scratch can start a crack that has nothing to do with the weld. Our lab prepares specimens to the dimensions in the code before bending, and we look at the surface before the test, not just after.
Before you weld the coupon
- Write the preliminary WPS with realistic parameters for the joint, not copied from another job.
- Check the bevel angle, root face and root gap before welding.
- Use the consumable and shielding gas the WPS names, and keep electrodes dry.
- Clean between every pass. Grind out anything that looks doubtful.
- Record the actual amps, volts, travel speed and interpass temperature – the PQR has to reflect what really happened.
If it fails anyway
Look at the fracture before throwing the coupon away. The shape and location of the opening usually tells you whether it was fusion, slag, root or preparation. That’s the information you need to change the procedure – otherwise the second coupon fails for the same reason as the first.
We can witness the qualification weld, test the coupon here in Guyana and talk you through any failure. That’s usually quicker than shipping coupons abroad and waiting.