Lot 319 Eccles Industrial Site, East Bank Demerara, Guyana · We work 24/7Phone/WhatsApp +592-602-5664 · Suriname +1-778 951 9480 · admin@kheeran.gy

Category: Welding

  • Hardness traverses across welds: when you need one and how to read it

    “We need a hardness traverse on the PQR.” It’s a line that turns up more and more in project specifications here, especially on anything that might see sour service or has been post-weld heat treated. If you haven’t had one done before, this is what it involves and why the client wants it.

    What a hardness traverse is

    A cross-section is cut through the weld, polished and etched so the weld metal, heat-affected zone and base metal are visible. Hardness readings are then taken in rows across the section – through the parent metal on one side, across the HAZ, through the weld and out the other side. Rows are usually placed near the cap, near the root and sometimes through the middle of the joint.

    Vickers (HV10) is the usual method because the small indent lets you place readings precisely in a narrow HAZ. The specification or code will say how many readings, where they go and how far apart.

    Why the HAZ matters most

    The heat-affected zone is the part of the base metal that was heated hot enough to change its structure but never melted. Next to the fusion line it can cool fast enough to form hard, brittle microstructures – especially in steels with a higher carbon equivalent or when preheat was too low. Hard zones are where hydrogen cracking and sulphide stress cracking start.

    That’s why the HAZ readings are the ones engineers look at first.

    Common limits

    For carbon and low-alloy steels in sour (H₂S) service, NACE MR0175 / ISO 15156 sets a maximum of 22 HRC, usually applied as 250 HV10 for weld procedure qualification. Many operators set their own limits, sometimes lower. For non-sour service, a typical project limit for carbon steel is somewhere around 325–350 HV10, but this varies – always check your specification rather than relying on a general number.

    When you’ll be asked for one

    • Procedure qualification for sour-service piping and pressure equipment
    • Procedures for higher-strength or higher-CE steels
    • Checking that post-weld heat treatment actually did its job
    • Repair procedures where a second heat cycle hits the original HAZ
    • Failure investigations, to see whether a hard zone played a part

    What to do if a reading is high

    First, look at where it is. A single high reading at the edge of the HAZ near the cap often points to fast cooling on the last pass – a temper bead technique or higher heat input may solve it. High readings across the whole HAZ suggest preheat was too low for the steel’s chemistry. High weld metal hardness can point to the consumable. PWHT will bring most carbon steel hardness down, but it adds cost and time, so it’s worth understanding the cause first.

    Our lab prepares the macro section, photographs it, runs the traverse and reports each reading on a sketch of the joint so you can see exactly where any high values sit.

    More about hardness and weld testing →

  • Why PQR bend tests fail – and how to avoid it

    A failed bend test on a procedure qualification record is painful. The coupon has been welded, cut and machined, the inspector has signed off on the parameters, and then a crack opens up on the convex face of the bend. Now you’re welding the whole thing again.

    We test a lot of PQR and welder qualification coupons, and the failures tend to have the same handful of causes. Most of them are avoidable.

    What the bend test is actually checking

    A guided bend stretches the weld and heat-affected zone well past yield. Sound metal stretches. Lack of fusion, slag and porosity don’t – they open up. Under ASME Section IX the usual acceptance rule is that no open discontinuity on the convex surface may exceed 3 mm (1/8 in) in any direction, with some allowance for cracks at the corners of the specimen. AWS D1.1 has similar but not identical rules, so check which code you’re working to.

    The usual causes of failure

    Lack of sidewall fusion

    This is the big one, especially in side bends on thicker plate. Side bends are required for thicker coupons – under ASME IX, from 19 mm (3/4 in) – and they’re very good at finding fill passes that didn’t wet into the bevel face. Narrow bevel angles, too little travel angle and too-low current on fill passes are the common culprits.

    Slag trapped between passes

    With SMAW and flux-cored processes, slag left in the toe of a previous pass gets buried by the next one. Proper interpass cleaning and grinding of sharp toes stops most of it.

    Root problems

    Root bends expose incomplete penetration and suck-back. Root opening, land and alignment need to be right before the first bead goes in. This is why fit-up inspection is worth doing on a qualification coupon.

    Specimen preparation

    Not every failure is a welding failure. Weld reinforcement must be removed flush, grinding marks should run along the specimen rather than across it, and sharp edges need a small radius. A deep transverse grinding scratch can start a crack that has nothing to do with the weld. Our lab prepares specimens to the dimensions in the code before bending, and we look at the surface before the test, not just after.

    Before you weld the coupon

    • Write the preliminary WPS with realistic parameters for the joint, not copied from another job.
    • Check the bevel angle, root face and root gap before welding.
    • Use the consumable and shielding gas the WPS names, and keep electrodes dry.
    • Clean between every pass. Grind out anything that looks doubtful.
    • Record the actual amps, volts, travel speed and interpass temperature – the PQR has to reflect what really happened.

    If it fails anyway

    Look at the fracture before throwing the coupon away. The shape and location of the opening usually tells you whether it was fusion, slag, root or preparation. That’s the information you need to change the procedure – otherwise the second coupon fails for the same reason as the first.

    We can witness the qualification weld, test the coupon here in Guyana and talk you through any failure. That’s usually quicker than shipping coupons abroad and waiting.

    More about welding inspection and qualification →