Lot 319 Eccles Industrial Site, East Bank Demerara, Guyana · We work 24/7Phone/WhatsApp +592-602-5664 · Suriname +1-778 951 9480 · admin@kheeran.gy

Author: Kheeran Offshore Team

  • Testing HDPE butt-fusion joints to ASTM F2634

    Polyethylene pipe is everywhere in Guyana now – water mains, drainage, slurry lines and industrial pipework. Most of it is joined by butt fusion: heat the pipe ends on a plate, press them together and let the joint cool under pressure. Done right, the joint is as strong as the pipe. Done wrong, it can look perfect from outside and still fail in a brittle way.

    That’s what ASTM F2634 testing is for.

    What ASTM F2634 covers

    ASTM F2634 is a laboratory method for testing PE butt-fusion joints using a tensile-impact approach. Strips are cut through the joint, so the fusion line sits in the middle of each specimen, and pulled apart at high speed. The test records the energy needed to break the specimen and – just as importantly – how it breaks.

    Ductile or brittle: the part that matters

    A good fusion joint fails in a ductile way. The material stretches and whitens before it breaks, often away from the fusion line. A poor joint tends to break cleanly at the fusion line with little stretching. Even if the energy number looks acceptable, a brittle break at the joint is a warning sign that the fusion process isn’t right.

    Why joints fail the test

    From the HDPE joints we’ve tested, the common causes are:

    • Heater plate temperature outside the range in the fusion procedure, or not checked with a calibrated thermometer.
    • Contamination on the pipe ends – dust, moisture or touching the faced surface with a glove.
    • Wrong interfacial pressure, often because drag pressure wasn’t measured and added.
    • Cooling time cut short to keep production moving.
    • Environmental conditions – wind and rain on an open site affect heating and cooling more than people expect.

    We tested one series of large-diameter joints that kept failing brittle at the fusion line over several rounds. Once the fusion parameters and site practice were tightened up, the joints failed in a ductile way and passed. The test didn’t just reject joints – it showed the contractor what to fix.

    When to test

    • To qualify a fusion procedure before production starts
    • To qualify fusion machine operators
    • As periodic production checks on long pipelines
    • When a joint is suspected after a field failure

    Our Georgetown lab cuts, prepares and tests HDPE fusion joints and reports the energy and failure mode for each specimen, with photographs. Getting a result locally means a failed procedure can be fixed before kilometres of pipe go in the ground.

    More about HDPE and material testing →

  • Hold points, witness points and why your ITP matters

    If you’ve worked on an oil & gas or major infrastructure job, you’ve seen an inspection and test plan – the ITP. It’s usually a long table with columns of letters: H, W, R, S, M. Fabricators sometimes treat it as paperwork for the client. It’s actually the most useful document on the job for avoiding arguments at handover.

    What an ITP does

    The ITP lists every inspection and test activity in the order the work happens: material receipt, cutting, fit-up, welding, NDT, dimensional checks, pressure testing, coating, final inspection and documentation. For each one it names the procedure or standard, the acceptance criteria, the record that will be produced, and who has to be involved.

    That last column is where the letters come in.

    Hold point (H)

    Work stops until the named party has inspected and released it. If the client’s inspector has a hold point on fit-up of a pressure-retaining weld, the welder doesn’t strike an arc until that inspector has seen the joint and signed off. Skipping a hold point is one of the quickest ways to get work rejected, regardless of how good it is.

    Witness point (W)

    The named party must be notified and given the chance to attend. If they don’t turn up after proper notice, work can continue. The notice period – often 24 or 48 hours – is written into the contract, so keep a record of when notifications were sent.

    Review (R), surveillance (S) and monitor (M)

    Review means the party checks the records rather than attending. Surveillance or monitoring means they may drop in at any time without stopping the work. Exact definitions vary between companies, so read the legend on each ITP.

    Where ITPs go wrong

    • Too generic. A template copied from another job lists tests that don’t apply and misses ones that do.
    • No acceptance criteria. “Visual inspection” without a code reference means everyone has a different idea of acceptable.
    • Notifications not tracked. When a witness point is missed, nobody can prove the notice was sent.
    • Records left to the end. Trying to assemble a dossier from memory after the job is finished almost always leaves gaps.

    How we help

    We prepare and review ITPs, attend hold and witness points as the third party or as the fabricator’s own QC, and keep the records together as the job progresses. When the steel is ready to ship, the dossier is ready too.

    More about our QA/QC inspection services →

  • Hardness traverses across welds: when you need one and how to read it

    “We need a hardness traverse on the PQR.” It’s a line that turns up more and more in project specifications here, especially on anything that might see sour service or has been post-weld heat treated. If you haven’t had one done before, this is what it involves and why the client wants it.

    What a hardness traverse is

    A cross-section is cut through the weld, polished and etched so the weld metal, heat-affected zone and base metal are visible. Hardness readings are then taken in rows across the section – through the parent metal on one side, across the HAZ, through the weld and out the other side. Rows are usually placed near the cap, near the root and sometimes through the middle of the joint.

    Vickers (HV10) is the usual method because the small indent lets you place readings precisely in a narrow HAZ. The specification or code will say how many readings, where they go and how far apart.

    Why the HAZ matters most

    The heat-affected zone is the part of the base metal that was heated hot enough to change its structure but never melted. Next to the fusion line it can cool fast enough to form hard, brittle microstructures – especially in steels with a higher carbon equivalent or when preheat was too low. Hard zones are where hydrogen cracking and sulphide stress cracking start.

    That’s why the HAZ readings are the ones engineers look at first.

    Common limits

    For carbon and low-alloy steels in sour (H₂S) service, NACE MR0175 / ISO 15156 sets a maximum of 22 HRC, usually applied as 250 HV10 for weld procedure qualification. Many operators set their own limits, sometimes lower. For non-sour service, a typical project limit for carbon steel is somewhere around 325–350 HV10, but this varies – always check your specification rather than relying on a general number.

    When you’ll be asked for one

    • Procedure qualification for sour-service piping and pressure equipment
    • Procedures for higher-strength or higher-CE steels
    • Checking that post-weld heat treatment actually did its job
    • Repair procedures where a second heat cycle hits the original HAZ
    • Failure investigations, to see whether a hard zone played a part

    What to do if a reading is high

    First, look at where it is. A single high reading at the edge of the HAZ near the cap often points to fast cooling on the last pass – a temper bead technique or higher heat input may solve it. High readings across the whole HAZ suggest preheat was too low for the steel’s chemistry. High weld metal hardness can point to the consumable. PWHT will bring most carbon steel hardness down, but it adds cost and time, so it’s worth understanding the cause first.

    Our lab prepares the macro section, photographs it, runs the traverse and reports each reading on a sketch of the joint so you can see exactly where any high values sit.

    More about hardness and weld testing →

  • Why PQR bend tests fail – and how to avoid it

    A failed bend test on a procedure qualification record is painful. The coupon has been welded, cut and machined, the inspector has signed off on the parameters, and then a crack opens up on the convex face of the bend. Now you’re welding the whole thing again.

    We test a lot of PQR and welder qualification coupons, and the failures tend to have the same handful of causes. Most of them are avoidable.

    What the bend test is actually checking

    A guided bend stretches the weld and heat-affected zone well past yield. Sound metal stretches. Lack of fusion, slag and porosity don’t – they open up. Under ASME Section IX the usual acceptance rule is that no open discontinuity on the convex surface may exceed 3 mm (1/8 in) in any direction, with some allowance for cracks at the corners of the specimen. AWS D1.1 has similar but not identical rules, so check which code you’re working to.

    The usual causes of failure

    Lack of sidewall fusion

    This is the big one, especially in side bends on thicker plate. Side bends are required for thicker coupons – under ASME IX, from 19 mm (3/4 in) – and they’re very good at finding fill passes that didn’t wet into the bevel face. Narrow bevel angles, too little travel angle and too-low current on fill passes are the common culprits.

    Slag trapped between passes

    With SMAW and flux-cored processes, slag left in the toe of a previous pass gets buried by the next one. Proper interpass cleaning and grinding of sharp toes stops most of it.

    Root problems

    Root bends expose incomplete penetration and suck-back. Root opening, land and alignment need to be right before the first bead goes in. This is why fit-up inspection is worth doing on a qualification coupon.

    Specimen preparation

    Not every failure is a welding failure. Weld reinforcement must be removed flush, grinding marks should run along the specimen rather than across it, and sharp edges need a small radius. A deep transverse grinding scratch can start a crack that has nothing to do with the weld. Our lab prepares specimens to the dimensions in the code before bending, and we look at the surface before the test, not just after.

    Before you weld the coupon

    • Write the preliminary WPS with realistic parameters for the joint, not copied from another job.
    • Check the bevel angle, root face and root gap before welding.
    • Use the consumable and shielding gas the WPS names, and keep electrodes dry.
    • Clean between every pass. Grind out anything that looks doubtful.
    • Record the actual amps, volts, travel speed and interpass temperature – the PQR has to reflect what really happened.

    If it fails anyway

    Look at the fracture before throwing the coupon away. The shape and location of the opening usually tells you whether it was fusion, slag, root or preparation. That’s the information you need to change the procedure – otherwise the second coupon fails for the same reason as the first.

    We can witness the qualification weld, test the coupon here in Guyana and talk you through any failure. That’s usually quicker than shipping coupons abroad and waiting.

    More about welding inspection and qualification →

  • Reading a mill test certificate: six checks before you accept steel

    A mill test certificate is the steel’s birth certificate. It says what the material is, where it came from and how it performed when it was made. On most jobs in Guyana the certificate arrives with the steel from overseas, and it’s tempting to file it and move on.

    Don’t. A few minutes with the certificate before the material goes into stock can save a very expensive conversation later. These are the six checks we run when a client asks us to verify material on receipt.

    1. Does the heat number match the steel?

    Every certificate is tied to a heat (or cast) number. That number should be stamped, stencilled or tagged on the plate, pipe or bar. If it isn’t on the material, or it doesn’t match the paper, the certificate doesn’t belong to that steel – no matter how good the numbers look.

    2. Is it the right type of certificate?

    Many projects call for an EN 10204 type 3.1 certificate, where the results come from tests on the actual product and are signed off by the manufacturer’s inspection department independent of production. A 2.2 document only reports typical results. If your specification says 3.1 or 3.2, a 2.2 isn’t a substitute.

    3. Grade, standard and edition

    “A36” and “A572 Grade 50” are different steels. So are API 5L PSL1 and PSL2. Check the grade, the standard and – where your specification is specific – the edition. Dual-certified material is common and fine, as long as both designations appear on the certificate.

    4. Chemistry, including carbon equivalent

    Compare each element against the limits in the material standard and any tighter limits in your project specification. For anything that will be welded, work out or check the carbon equivalent. A high CE means more preheat and more risk of hydrogen cracking, and it should be reflected in the welding procedure.

    5. Mechanical properties

    Yield, tensile and elongation should sit inside the specified range – not just above the minimum. Some specs also cap yield-to-tensile ratio. If impact testing is required, check the test temperature as well as the energy values. A good result at 0 °C doesn’t satisfy a –20 °C requirement.

    6. Supplementary requirements and heat treatment

    Normalised, quenched and tempered, sour-service hardness limits, through-thickness (Z) properties, ultrasonic testing of plate – if your purchase order asked for it, it should be on the certificate. Missing supplementary requirements are the most common gap we find.

    When the certificate isn’t enough

    Sometimes the paperwork is missing, illegible or doesn’t match the steel. That doesn’t always mean the material has to be scrapped. Verification testing – chemical analysis plus tensile and, if needed, impact tests on samples from the actual material – can establish what you have. Whether the result is acceptable is then a decision for your engineer and your client, but at least it’s based on facts.

    We do this kind of verification testing in our Georgetown laboratory regularly. If you’ve got material with doubtful paperwork, get in touch before it gets welded in.

    See our material testing services →

  • One low Charpy result: what it means and what to do next

    You’ve sent a set of three Charpy specimens to the lab. Two come back comfortably above the minimum. The third is well below it. The steel is already cut, the fabricator wants to start welding, and somebody asks the obvious question: does the plate fail?

    Not necessarily. But you shouldn’t wave it through either. Here’s how we think about a single low Charpy value when it lands on our desk in Eccles.

    Charpy results scatter more than people expect

    Impact testing measures how much energy a small notched bar absorbs when a pendulum breaks it. That bar is 10 mm square and the notch is 2 mm deep, so you are sampling a tiny volume of steel. If that volume happens to include a stringer of inclusions, a band of harder microstructure or, in a weld, a coarse-grained patch of heat-affected zone, the number drops. Move the notch a millimetre and you can get a very different answer.

    That’s why most specifications don’t judge on a single specimen. They ask for a set of three and set two limits: a minimum average for the set, and a lower minimum for any one specimen – often around two-thirds of the average requirement. Check your own specification for the exact figures, because they vary between material standards, codes and project specs.

    First, rule out the test itself

    Before blaming the steel, make sure the low value is real. These are the things we check:

    • Temperature. For sub-zero tests the specimen has to be broken within a few seconds of leaving the cooling bath. ASTM E23 allows five seconds. A slow transfer at –20 °C or below can shift results.
    • Notch. A notch with a worn tool or the wrong radius concentrates stress differently. We check notch geometry before testing, not after.
    • Notch location. In weld tests, “HAZ” covers a band a few millimetres wide. If the procedure says fusion line plus 2 mm and the notch drifted into weld metal, you’re testing something else.
    • Specimen size. Sub-size specimens have their own, lower acceptance values. Comparing a 7.5 mm specimen against a full-size requirement makes a good result look bad.
    • The fracture face. We look at every broken specimen. A visible defect on the fracture face – porosity, a slag line, lack of fusion – tells you the low value is about that defect, not the base material’s toughness.

    Then check what the specification allows

    Many product specifications allow a retest when the set average passes but one specimen falls below the single-value minimum. A common rule is that three more specimens are taken from the same location, and each of them must meet the required average on its own. That’s a much harder bar than the first set, which is deliberate.

    Some project specifications don’t allow retests at all, or require the client’s approval first. Read the spec before cutting new specimens, not after.

    What we’d do with your low value

    1. Confirm the test conditions and photograph the fracture faces.
    2. Report all three values exactly as measured, with lateral expansion and shear area if your spec asks for them.
    3. Note anything visible on the fracture surface.
    4. If the spec allows a retest, prepare the new specimens from material next to the original ones and test them – ideally with your inspector watching.

    What we won’t do is quietly retest until we get a better number. A Charpy report is only useful if every result is on it.

    The short version

    One low value is a reason to look closer, not an automatic rejection. Check the test, read the specification, retest where it’s allowed, and keep every result on the record. If you’d like a second opinion on a set of results, send them through. We’re always happy to look.

    More about our Charpy and mechanical testing →