You’ve sent a set of three Charpy specimens to the lab. Two come back comfortably above the minimum. The third is well below it. The steel is already cut, the fabricator wants to start welding, and somebody asks the obvious question: does the plate fail?
Not necessarily. But you shouldn’t wave it through either. Here’s how we think about a single low Charpy value when it lands on our desk in Eccles.
Charpy results scatter more than people expect
Impact testing measures how much energy a small notched bar absorbs when a pendulum breaks it. That bar is 10 mm square and the notch is 2 mm deep, so you are sampling a tiny volume of steel. If that volume happens to include a stringer of inclusions, a band of harder microstructure or, in a weld, a coarse-grained patch of heat-affected zone, the number drops. Move the notch a millimetre and you can get a very different answer.
That’s why most specifications don’t judge on a single specimen. They ask for a set of three and set two limits: a minimum average for the set, and a lower minimum for any one specimen – often around two-thirds of the average requirement. Check your own specification for the exact figures, because they vary between material standards, codes and project specs.
First, rule out the test itself
Before blaming the steel, make sure the low value is real. These are the things we check:
- Temperature. For sub-zero tests the specimen has to be broken within a few seconds of leaving the cooling bath. ASTM E23 allows five seconds. A slow transfer at –20 °C or below can shift results.
- Notch. A notch with a worn tool or the wrong radius concentrates stress differently. We check notch geometry before testing, not after.
- Notch location. In weld tests, “HAZ” covers a band a few millimetres wide. If the procedure says fusion line plus 2 mm and the notch drifted into weld metal, you’re testing something else.
- Specimen size. Sub-size specimens have their own, lower acceptance values. Comparing a 7.5 mm specimen against a full-size requirement makes a good result look bad.
- The fracture face. We look at every broken specimen. A visible defect on the fracture face – porosity, a slag line, lack of fusion – tells you the low value is about that defect, not the base material’s toughness.
Then check what the specification allows
Many product specifications allow a retest when the set average passes but one specimen falls below the single-value minimum. A common rule is that three more specimens are taken from the same location, and each of them must meet the required average on its own. That’s a much harder bar than the first set, which is deliberate.
Some project specifications don’t allow retests at all, or require the client’s approval first. Read the spec before cutting new specimens, not after.
What we’d do with your low value
- Confirm the test conditions and photograph the fracture faces.
- Report all three values exactly as measured, with lateral expansion and shear area if your spec asks for them.
- Note anything visible on the fracture surface.
- If the spec allows a retest, prepare the new specimens from material next to the original ones and test them – ideally with your inspector watching.
What we won’t do is quietly retest until we get a better number. A Charpy report is only useful if every result is on it.
The short version
One low value is a reason to look closer, not an automatic rejection. Check the test, read the specification, retest where it’s allowed, and keep every result on the record. If you’d like a second opinion on a set of results, send them through. We’re always happy to look.